Effect of Hydrofluoric Acid Surface Treatments on Surface Roughness and Three-Point Flexural Strength of Suprinity Ceramic

Abstract

Objectives: This study aimed to evaluate the effects of hydrofluoric acid (HF) concentration and etching time on the surface roughness (SR) and three-point flexural strength of Suprinity and to analyze the surface elements before and after etching.
Materials and Methods: To measure the SR, 70 specimens of Suprinity (2×4×5mm3) were assigned to seven groups (n=10). Six groups were etched for 20, 60, and 120 seconds with 5% and 10% HF and 7th group was the control group. Specimens were evaluated using atomic force microscopy (AFM). One specimen from each group was used to analyze the surface elements using scanning electron microscopy (SEM). For measuring the three-point flexural strength, 60 specimens were divided into six groups (n=10) and etched as previously described. The flexural strength was measured using a universal testing machine. T-test, one-way analysis of variance (ANOVA), and two-way ANOVA were used for statistical analyses (P<0.05).
Results: The 10% concentration of HF caused higher SR compared to the 5% HF. The effect of HF concentration on the flexural strength was significantly different in the 20- and 60-second etching groups. Different etching times had no significantly different effect on the SR. With 5% HF, the flexural strength was significantly higher for 20-second etching time than for the etching times of 60 and 120 seconds. With 10% HF, there was a significant difference in flexural strength between etching times of 20 and 120 seconds. 
Conclusions: The best surface etching protocol comprises 10% HF used for 20 seconds.

- Zogheib L.V, Della Bona A. Effect of hydrofluoric acid etching duration on the roughness and flexural strength of a lithium disilicate-based glass ceramic. Braz Dent J. 2011; 22(1):45-50.

- Wai Kim Li.R, Chow T.W, Matinlinna J.P. Ceramic dental biomaterials and CAD/CAM technology: State of the art. Journal of prosthodontic research .2014; 58: 208 – 216.

- Manhart J, Chen H, Hamm G, Hickel R. Buonocore Memorial Lecture. Review of the clinical survival of direct and indirect restorations in posterior teeth of the permanent dentition. Oper Dent.2004; 29: 481–508.

- MokhtarpourF,Alaghehman H. Effect of hydrofluoric acid surface treatments on micro-shear bond strength of CAD/CAM ceramics. Electronic Physician jurnal.2017;9(10):5487-5493

- Özcan M,Vallittu PK. Effect of surface conditioning methods on the bond strength of luting cement to ceramics. Dent Mater. 2003; 19(8): 725–31.

- Horn HR. Porcelain laminate veneers bonded to etched enamel. Dental Clinics of North America, 1983; 27(4): 671–684.

- Malament KA, Socranski SS. Survival of Dicor glass-ceramic dental restorations over 16 years. Part III. Effect of luting agent and tooth or tooth-substitute core structure. Journal of Prosthetic Dentistry. 2001; 86(5): 511-519.

- ProchnowC,VentoriniAB. Effect of etching with distinct hydrofluoric acid concentrations on the flexural strength of a lithium disilicate-basedglassceramic. Journal of biomaterials research Part B; 2017; 105:885-891.

- Chen JH, Matsumura H, Atsuta M. Effect of different etching periods on the bond strength of a composite resin to a machinable porcelain. J Dent. 1998; 26(1): 53-8.

- Bona A D, Anusavice KJ, DeHoff PH. Weibull analysis and flexural strength of hot pressed core and veneered ceramic structures. Dent Mater 2003; 19(7):662–669.

- ElsakaSE ,ElnaghyA M. Mechanical properties of zirconia reinforced lithium silicate glass-ceramic. Dental materials 2016; 32(7):908-914.

- MclarenEA, FiqueiralJ. Updating classification of ceramic dental materials: A guide to material selection. CompendContinEduc Dent . 2015; 36(6):400-405.

- RamosNde C, Campos TM, Machado JP. Microstructure characterization and SCG of newly engineered dental ceramics. Dental Materials.2016; 32(7):870-878.

- Lu R, Harcourt JK, Tyas MJ, Alexander B. An investigation of the composite resin/porcelain interface. Aust Dent J. 1992; 37: 12-9.

- Nagayassu MP, Shintome LK, Uemura ES, Araujo JE. Effect of Surface Treatment on the Shear Bond Strength of a Resin-Based Cement to Porcelain. Braz Dent J. 2006; 17(4): 290-5.

- Ramakrishnaiah R,Alkheraif AA, DarshanD. The effect of hydrofluoric acid etching duration on the surface micromorphology, roughness and wettability of dental ceramics. Int.J.Mol.Sa. 2016, 17(6), pii: E822.

- Stangel I,Nathanson D, Hsu CS. Shear strength of the composite bond to etched porcelain. J Dent Res. 1987; 66(9): 1460–5.

-Vita Suprinity CAD/CAM Restorative. Vita Suprinity Brochure. Available at: https://www.vita-zahnfabrik.com/en/VITA-SUPRINITY-14036.html

-YenTW,Black man R, Baez RJ. Effect of acid etching on the flexural strength of a feldespatic porcelain and a castable glass ceramic. Journal of Prosthetic Dentistry.1993, 70(3); 224-233.

- Addison O, Marquis P.M. The impact of hydrofluoric acid surface treatments on the performance of a porcelain laminate restorative material. Dental Materials 2007;23 (4):461–468.

- Sato, TP. Yamamoto, L.T, Rossi, N.R.; Macedo, V.C.; Kimpara, E.T. Flexural strength of a pressable lithium disilicate ceramic: influence of surface treatments. Appl. Adhesion Sci.2013, 1, 1–7.

- Bertin,Eugene P. Introduction to X-ray spectrometric analysis; Springer Science & Business Media, New York (NY), 2013.ISBN:978-1-4899-2204-5

Files
IssueVol 17 (Continuously Published Article-Based) QRcode
SectionOriginal Article
DOI https://doi.org/10.18502/fid.v17i22.4316
Keywords
Glass Ceramic VITA Suprinity Hydrofluoric Acid Surface Properties Flexural Strength

Rights and permissions
Creative Commons License This work is licensed under a Creative Commons Attribution-NonCommercial 4.0 International License.
How to Cite
1.
Keshmiri N, Alaghehmand H, Mokhtarpour F. Effect of Hydrofluoric Acid Surface Treatments on Surface Roughness and Three-Point Flexural Strength of Suprinity Ceramic. Front Dent. 2020;17.